Optical Lithography Resources: Difference between revisions
| Line 17: | Line 17: | ||
Resist, parameters, notes | Resist, parameters, notes | ||
==Positive== | |||
{| class="wikitable sortable" style="text-align: center;" | {| class="wikitable sortable" style="text-align: center;" | ||
| Line 23: | Line 25: | ||
|- | |- | ||
| S1813 || Dehydrate on hot plate || 2000rpm || 1um || 100C 1min || 12s || - || - || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | | S1813 || Dehydrate on hot plate || 2000rpm || 1um || 100C 1min || 12s || - || - || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | ||
|- | |||
| AZ5214 || Dehydrate on hot plate || 2000rpm || 1um || 100C 1min || 25s || - || - || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | |||
|} | |||
==Negative== | |||
{| class="wikitable sortable" style="text-align: center;" | |||
|- | |||
! Resist !! Wafer Prep !! Spin !! Thickness !! Prebake !! Exposure !! Postbake !! Flood !! Development !! Hardbake !! Lamp !! Notes | |||
|- | |- | ||
| AZ5214 || Dehydrate on hot plate || 2000rpm || 1um || 100C 1min || 12s || 110C 1min || 30s || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | | AZ5214 || Dehydrate on hot plate || 2000rpm || 1um || 100C 1min || 12s || 110C 1min || 30s || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | ||
Revision as of 03:22, 4 November 2019
Trove of lithography application notes:
https://www.microchemicals.com/downloads/application_notes.html
troubleshooting, photoresist procedures, liftoff, etching, etc.
KNI Photoresists
List of KNI Photoresists
- S1813 standard positive, withstands acid etching
- AZ5214, positive and image reversal negative, good for liftoff
Table of photoresist recipes from KNI papers:
Resist, parameters, notes
Positive
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|
| S1813 | Dehydrate on hot plate | 2000rpm | 1um | 100C 1min | 12s | - | - | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 (Link KNI recipe doc here) |
| AZ5214 | Dehydrate on hot plate | 2000rpm | 1um | 100C 1min | 25s | - | - | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 (Link KNI recipe doc here) |
Negative
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ5214 | Dehydrate on hot plate | 2000rpm | 1um | 100C 1min | 12s | 110C 1min | 30s | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 (Link KNI recipe doc here) |
SU8 Guide
BYU SU-8 Guide https://cleanroom.byu.edu/su8
Sizes provided by KNI: 2050, 2005, 2001, 2000.5
Other Photoresists
resist list https://cleanroom.byu.edu/resistmanufacturers
UCSB photoresist recipes:
https://www.nanotech.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes
https://www.nanotech.ucsb.edu/wiki/index.php/Contact_Alignment_Recipes
BYU Photoresist recipes https://cleanroom.byu.edu/photoresists
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Developer | Development | Hardbake | Mask Aligner | Wattage | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| nLoF 2070 | Dehydrate on hot plate | 2000rpm | 7um | 100C 5min | 120s | - | - | MF319 | 120s | - | Suss1 Ch1 | 15mW/cm^2 | Measured 10/19 (Link KNI recipe doc here) |
Photolithography Resources
Link to BYU photolithograph https://cleanroom.byu.edu/processes#Microfab_PhotoLith
link to definitions: https://kayakuam.com/techreferences/lithography-terms/ https://cleanroom.byu.edu/definitions
resolution https://pages.mtu.edu/~microweb/chap1/ch1-4-1.htm