Optical Lithography Resources: Difference between revisions

From the KNI Lab at Caltech
Jump to navigation Jump to search
Line 54: Line 54:
=Other Photoresists=
=Other Photoresists=


resist list
*[https://cleanroom.byu.edu/resistmanufacturers BYU Comprehensive list of photoresists]
https://cleanroom.byu.edu/resistmanufacturers


UCSB photoresist recipes:
*[https://www.nanotech.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes UCSB Photoresist Recipes Page 1]


https://www.nanotech.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes
*[https://www.nanotech.ucsb.edu/wiki/index.php/Contact_Alignment_Recipes UCSB Photoresist Recipes Page 2]
 
https://www.nanotech.ucsb.edu/wiki/index.php/Contact_Alignment_Recipes
 
BYU Photoresist recipes
https://cleanroom.byu.edu/photoresists


*[https://cleanroom.byu.edu/photoresists BYU Photoresist Recipes]


==Non-KNI Photoresist Recipes]]
{| class="wikitable sortable" style="text-align: center;"
{| class="wikitable sortable" style="text-align: center;"
|-
|-
! Resist !! Wafer Prep !! Spin !! Thickness !! Prebake !! Exposure !! Postbake !! Flood !! Developer  !! Development  !! Hardbake !! Mask Aligner !! Wattage !! Notes  
! Resist !! Wafer Prep !! Spin !! Thickness !! Prebake !! Exposure !! Postbake !! Flood !! Development  !! Hardbake !! Lamp !! Notes  
|-
|-
| nLoF 2070 || Dehydrate on hot plate || 2000rpm || 7um || 100C 5min || 120s || - || - || MF319 || 120s || - || Suss1 Ch1 || 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here)
| nLoF 2070 || Dehydrate on hot plate || 2500rpm || 7um || 110C 90s || 12s || 110C 90s || - || AZ 729 2min || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19
|-
|-
|}
|}

Revision as of 05:07, 4 November 2019

Template:NOINDEX

Trove of lithography application notes from MicroChemicals covering troubleshooting, procedures, techniques, theory

KNI Photoresists

Photoresists provided by KNI:

  • S1813: standard positive, withstands acid etching
  • AZ5214: positive and image reversal negative, good for liftoff
  • SU-8: thick polymer structures

Positive Photoresist Recipes

See recipe notes for additional information on wafer cleaning and prep, edge bead removal, and spin curves.

Resist Wafer Prep Spin Thickness Prebake Exposure Postbake Flood Development Hardbake Lamp Notes
S1813 Dehydrate on hot plate 3000rpm 1.5um 115C 1min X - - X - Suss1 Ch1 15mW/cm^2 Measured 10/19 (Link KNI recipe doc here)
AZ5214 Dehydrate on hot plate 2000rpm 1um 100C 1min 25s - - MF319 60s - Suss1 Ch1 15mW/cm^2 Measured 10/19

Negative Photoresist Recipes

See recipe notes for additional information on wafer cleaning and prep, edge bead removal, and spin curves.

Resist Wafer Prep Spin Thickness Prebake Exposure Postbake Flood Development Hardbake Lamp Notes
AZ5214 Dehydrate on hot plate 2000rpm 1.8um 100C 1min 12s 110C 1min 40s MF319 60s - Suss1 Ch1 15mW/cm^2 Measured 10/19
Dehydrate on hot plate 3500rpm 1.4um 100C 1min 9s 110C 1min 30s MF319 60s - Suss1 Ch1 15mW/cm^2 Measured 10/19

SU-8 Recipes

SU-8 is available in thicknesses ranging from 500nm to 500microns. Remember to use Laurel Spinner 1.

Resist thicknesses currently provided by KNI: 2050, 2005, 2001, 2000.5

BYU SU-8 Guide

Resist Wafer Prep Spin Thickness Prebake Exposure Postbake Development Hardbake Lamp Notes
2050 Dehydrate on hot plate 3000rpm 50um 65C 3min 95C 9min X 65C 2min 95C 7min SU-8 Developer X seconds Optional Suss1 Ch1 15mW/cm^2 Measured 10/19

Other Photoresists

==Non-KNI Photoresist Recipes]]

Resist Wafer Prep Spin Thickness Prebake Exposure Postbake Flood Development Hardbake Lamp Notes
nLoF 2070 Dehydrate on hot plate 2500rpm 7um 110C 90s 12s 110C 90s - AZ 729 2min - Suss1 Ch1 15mW/cm^2 Measured 10/19

Photolithography Resources

Link to BYU photolithograph https://cleanroom.byu.edu/processes#Microfab_PhotoLith

link to definitions: https://kayakuam.com/techreferences/lithography-terms/ https://cleanroom.byu.edu/definitions

resolution https://pages.mtu.edu/~microweb/chap1/ch1-4-1.htm